Loss of Mass, 110-1000°C as H 2O and C
|
|
n/a |
9,6 ± 0,1 |
% |
LECO or TGA |
|
|
|
n/a |
20,1 ± 0,2 |
% |
Alcan SM 1359-99, XRF, glass beads/ICP |
|
Iron (Fe) as Fe2O3
|
|
n/a |
44,2 ± 0,5 |
% |
Alcan SM 1359-99, XRF, glass beads/ICP |
|
Silicon (Si) as SiO2
|
|
n/a |
10,3 ± 0,1 |
% |
Alcan SM 1359-99, XRF, glass beads/ICP |
|
Titanium (Ti) as TiO2
|
|
n/a |
6,99 ± 0,05 |
% |
Alcan SM 1359-99, XRF, glass beads/ICP |
|
Cr2O3
|
|
n/a |
0,181 ± 0,003 |
% |
Alcan SM 1359-99, XRF, glass beads/ICP |
|
Calcium (Ca) as CaO
|
|
n/a |
1,15 ± 0,02 |
% |
Alcan SM 1359-99, XRF, glass beads/ICP |
|
Phosphorus (P)as P2O5
|
|
n/a |
0,198 ± 0,005 |
% |
Alcan SM 1359-99, XRF, glass beads/ICP |
|
ZrO2
|
|
n/a |
0,213 ± 0,006 |
% |
Alcan SM 1359-99, XRF, glass beads/ICP |
|
Zinc (Zn) as ZnO
|
|
n/a |
0,007 ± 0,002 |
% |
Alcan SM 1359-99, XRF, glass beads/ICP |
|
Manganese (Mn) as MnO2
|
|
n/a |
0,019 ± 0,004 |
% |
Alcan SM 1359-99, XRF, glass beads/ICP |
|
Vanadium (V) as V2O5
|
|
n/a |
0,210 ± 0,004 |
% |
Alcan SM 1359-99, XRF, glass beads/ICP |
|
Potassium as K2O
|
|
n/a |
0,032 ± 0,004 |
% |
Alcan SM 1359-99, XRF, glass beads/ICP |
|
|
|
[1309-48-4] |
0,049 ± 0,008 |
% |
Alcan SM 1359-99, XRF, glass beads/ICP |
|
Sodium (Na) as Na2O
|
|
n/a |
6,1 ± 0,1 |
% |
Alcan SM 1359-99, XRF, glass beads/ICP |
|
Sulfur as % SO3
|
|
n/a |
0,44 ± 0,02 |
% |
|
|
g-Al2O3 as Al2O3
|
|
n/a |
1,4 ± 0,2 |
% |
DSC Alcan SM 1029-00 |
|
Total Extratable Alumina as Al2O3
|
|
n/a |
9,8 ± 0,1 |
% |
Alcan SM 1177-04 , high temperature digestion1 |
|
Total Organic Carbon
|
|
n/a |
0,23 ± 0,03 |
% |
Wet Oxidation |
|